Expulsion at Weld Interface
- Short Squeeze Time
- Low Weld Force
- Dirty – Scaly Material
- Poor Fit Up
- Insufficient Edge Distance
Surface Expulsion/Electrode Sticking
- Short Squeeze Time
- Long Weld Time
- Short Hold Time
- Low Weld Force
- High Weld Current
- Dirty - Scaly Material
Electrode Mushrooming
- Insufficient Cooling
- Low weld Force
- High Weld Current
- Small Electrode Face Area
- Long Weld Time
- Welder Head Impacts Work
Low Weld Strength
- Short Weld Time
- Low Weld Force
- Low Weld Current
- Small Electrode Face Area
- Poor Heat Balance
- Welds Too Close Together
Excessive Weld Indentation
- Long Weld Time
- High Weld Force
- High Weld Current
- Poor Fit Up
- Welder Head Impacts Work
Internal Cracks in Weld Nugget
- Short Hold Time
- Low Weld Force
- Dirty- Scaly Material
- Metallurgy of Material Welded
- Poor Head Follow Up
Displaced Weld Nugget
- Electrode Misalignment
- Poor Heat Balance
- Poor Fit UP
Cracks in Parent Material
- High Weld Force
- Insufficient Cooling
- Metallurgy of Material Welded